Table 1 Thermal degradation temperature (T d) andT 5of MWCNTs/polyimide nanocomposites

From: Influence of Surface Modified MWCNTs on the Mechanical, Electrical and Thermal Properties of Polyimide Nanocomposites

Temperature (°C)

Pure PI

Acid-MWCNTs/polyimide (MWCNTs wt%)

Amide-MWCNTs/polyimide (MWCNTs wt%)

0.5

1

2

3

5

0.5

1

2

3

5

*T d

510

515

530

540

570

555

525

520

520

525

525

**T 5

540

545

555

565

585

580

553

550

550

550

550

  1. * Temperature at which degradation starts
  2. ** Temperature at which 5 wt% of the material has degraded