Skip to main content
Account

Table 6 Thermal degradation data of various EVA nanocomposites at 4 wt% filler loading

From: Influence of Matrix Polarity on the Properties of Ethylene Vinyl Acetate–Carbon Nanofiller Nanocomposites

Sample

TMax(°C)

Maximum rate of degradation (%/°C)

EVA40

453

2.24

EVA50

462

1.78

EVA60

483

1.47

EVA70

486

1.23

EVA40-4EG

469

1.72

EVA50-4EG

476

1.53

EVA60-4EG

498

1.47

EVA70-4EG

498

1.12

EVA40-4T

460

1.37

EVA50-4T

466

1.48

EVA60-4T

488

1.44

EVA70-4T

487

1.06

EVA40-4F

456

2.39

EVA50-4F

470

1.55

EVA60-4F

491

1.38

EVA70-4F

493

1.08