Table 1 Physical properties of the prepared mesoporous sulphated silica-zirconia materials
Sample | Added Zr (wt.%) | Zr loadinga(wt.%) | Si/Zr (mol/mol) | Sulphur loadingb(wt.%) | Zr/S | Surface area (m2/g) | Pore volume (cm3/g) | Pore diameter (Å) |
---|---|---|---|---|---|---|---|---|
1 | - | - | ∞ | - | - | 709 | 0.819 | 46.15 |
2 | 2.2 | 1.01 | 148 | 0.05 | 7.1 | 435 | 1.343 | 123.52 |
3 | 3.6 | 1.34 | 111 | 0.10 | 4.7 | 416 | 1.291 | 124.23 |
4 | 7.9 | 2.43 | 60 | 0.33 | 2.6 | 482 | 1.166 | 96.89 |
5 | 10.9 | 5.29 | 27 | 0.28 | 6.6 | 470 | 1.075 | 91.47 |
6 | 25.0 | 15.35 | 7.8 | 0.73 | 7.4 | 424 | 1.167 | 110.08 |
7 | 39.5 | 26.89 | 3.6 | 1.08 | 8.8 | 378 | 0.763 | 80.73 |
8 | 45.0 | 27.77 | 3.4 | 1.22 | 8.0 | 380 | 0.558 | 58.63 |
9 | 61.5 | 41.40 | 1.6 | 1.69 | 8.6 | 343 | 0.430 | 50.23 |