Skip to main content

Table 1 Summary of post growth nitridation conditions used for the conversion of ZnO into Zn3N2 NWs

From: The nitridation of ZnO nanowires

  T N
(°C)
NH3
(sccm)
t N
(min)
Ramp rate (°C/min)
CVD1196 500 250 60 30
CVD1198 550 250 60 30
CVD1194 600 250 60 30
CVD1197 630 250 60 30
CVD1195 700 250 60 30
CVD1199 600 50 60 30
CVD1217 600 500 60 30
CVD1214 600 250 90 30
CVD1218 600 250 120 30
CVD1200 600 250 60 10
CVD1211 600 500 60 10
  1. TN, nitridation temperature; tN, nitridation time.