Table 2 Effect of different modifications of AAO pores on fringe intensity

From: Controlling interferometric properties of nanoporous anodic aluminium oxide

Coating material

AAO

Pt

Au

Cr

Ni

Ag

TiO2 (ALD)

Thickness (nm)

 

8

8

9

5

13

10

Interference maximum intensitya (a.u.)

10 ± 3

50 ± 5

98 ± 6

100 ± 8

65 ± 2

35 ± 2

11 ± 2

  1. aAverage of five measurements plus standard deviation. AAO, anodic aluminium oxide; ALD, atomic layer deposition; a.u., arbitrary unit.