Table 1 Characteristics of DSSCs composed of the compressed TiO 2 NP thin film as photoanode
Sample | Thickness | R K | V OC | J SC | FF | η |
---|---|---|---|---|---|---|
(μm) | (Ω) | (V) | (mA/cm2) | (%) | (%) | |
A | 12.7 | 19.2 | 0.71 | 12.62 | 60.89 | 5.43 |
B | 14.2 | 12.5 | 0.68 | 19.88 | 57.90 | 7.80 |
C | 25.0 | 10.6 | 0.68 | 21.59 | 58.33 | 8.59 |
D | 26.6 | 9.41 | 0.68 | 22.41 | 59.66 | 9.01 |
E | 35.3 | 9.87 | 0.66 | 22.32 | 56.10 | 8.30 |
F | 55.2 | 10.1 | 0.62 | 19.37 | 54.67 | 5.85 |