Table 3 Experimental parameters of the DSSC-type solar cells relative to the paste used to deposit the porous TiO2 film
From: Effect of Anatase Synthesis on the Performance of Dye-Sensitized Solar Cells
Synthesis pressure (atm) | Paste | V OC (V) | J SC (mA cm−2) | FF | η% |
---|---|---|---|---|---|
4 | A127 | 0.71 | 6.04 | 0.65 | 2.84 |
9.5 | A148 | 0.73 | 6.75 | 0.68 | 3.38 |
19.5 | A167 | 0.66 | 9.51 | 0.66 | 4.21 |