Skip to main content
Account

Table 1 Photovoltaic parameters of DSSCs with nanostructured ZnO photoanodes under simulated AM 1.5 G light illumination

From: Room Temperature Deposition of Crystalline Nanoporous ZnO Nanostructures for Direct Use as Flexible DSSC Photoanode

A

 

J sc (mA cm−2)

V oc (V)

FF (%)

η (%)

100 mTorr

508

0.44

51

1.58

200 mTorr

11.4

0.57

50

3.23

300 mTorr

13.1

0.55

54

3.89

400 mTorr

12.7

0.53

51

3.41

B

2.5 μm

4.3

0.60

49

4.27

5.0 μm

8.5

0.57

50

2.43

7.5 μm

11

0.57

57

3.58

10.0 μm

13.1

0.55

54

3.89

15.0 μm

13.7

0.56

50

3.86

Flexible 10 μm

10.8

0.55

57

3.4

  1. J sc, V oc, FF, and η denote saturated photocurrent, open circuit voltage, fill factor, and overall efficiency, respectively
  2. A as a function of ambient oxygen pressure for ZnO deposition (the thicknesses of all the ZnO films were fixed to be 10 μm)
  3. B as function of film thickness (all films were deposited under 300 mTorr)

Navigation