Table 1 Spinning parameters for preparing PAN and PVP nanofibers

From: Influence of Working Temperature on The Formation of Electrospun Polymer Nanofibers

No.

Working fluida

Temperature (°C)

Other conditionsb

Polymer

Solvent

Applied voltage

Flow rate

F1

PAN

(Con. 15%)

DMAc

(BP:166.0)

20 ± 1

14 kV

1 mL/h

F2

40 ± 1

F3

60 ± 2

F4

80 ± 2

F5

PVP K90

(Con. 9%)

Ethanol

(BP:78.5)

20 ± 1

10 kV

2 mL/h

F6

30 ± 1

F7

40 ± 1

F8

50 ± 1

F9

60 ± 2

  1. aCon. means concentration in w/v, and BP means boiling point in °C
  2. bThe fiber-collected distance was fixed at 15 cm