Skip to main content
Account

Table 3 TGA data obtained for CER-based networks and pure [HPyr][BF4]

From: Nanoporous Polymer Films of Cyanate Ester Resins Designed by Using Ionic Liquids as Porogens

Samples

T d1 a (°C)

T dmax b (°C)

T d50% c (°C)

Mass loss at T dmax (%)

Char residue (wt%)

CER

425

435

694

16

50

CER20ext

399

435

538

32

42

CER30ext

396

434

528

33

42

CER40ext

395

435

503

35

40

CER40

340

385

393

42

25

[HPyr][BF4]

376

416

407

67

2

  1. aOnset temperature of intensive degradation as determined by value for intersection of tangents to curve at the first inflection point
  2. bTemperature value of maximal degradation rate
  3. cTemperature values for a 50% mass loss