Table 1 Parameters used in AuNP synthesis for each experiment

From: Gold nanoparticles with chitosan, N-acylated chitosan, and chitosan oligosaccharide as DNA carriers

Experiment

Average MW chitosan (Da)

Chitosan (wt%)

HAuCl4∙3H2O concentration (wt%)

Temperature (°C)

Time (min)

CO-AuNPsa

120000

0.12

0.100

25

150

Acyl-CO-AuNPsb

120000

0.69

0.100

25

90

COS@1-AuNPsc

5000

0.99

0.003

80

60

COS@2-AuNPsd

5000

1.96

0.003

80

60

COS@3-AuNPse

5000

0.99

0.017

80

60

COS@4-AuNPsf

5000

1.96

0.017

80

60