Table 1 Physicochemical parameters derived from nitrogen physisorption and XRD datas for different samples (d100is the interplanar spacing of the hexagonal structure;a0represents the pore-to-pore distance of the hexagonal structure)

From: Structure and Photoluminescent Properties of ZnO Encapsulated in Mesoporous Silica SBA-15 Fabricated by Two-Solvent Strategy

Samples

d100(nm)

a0(nm)

SBET(m2/g)

Pore diameter (nm)

Pore volume (cm3/g)

Extracted SBA-15

10.5

12.1

807

6.41

0.985

8 wt% ZnO/SBA-15

9.9

11.4

683

6.11

0.921

15 wt% ZnO/SBA-15

10.0

11.6

564

6.07

0.794

20 wt% ZnO/SBA-15

10.3

11.9

498

6.04

0.716