Skip to main content
Account

Table 1 Properties of prepared LSMO

From: Magnetic and Cytotoxicity Properties of La1−xSr x MnO3(0 ≤ x ≤ 0.5) Nanoparticles Prepared by a Simple Thermal Hydro-Decomposition

La1−xSr x MnO3

Thermally decomposed in the range of 700 → 900°C for 6 h

Sr content

0

0.1

0.2

0.3

0.4

0.5

Crystal structure

Cubic Rhombo

Cubic Rhombo

Cubic Rhombo

Cubic Rhombo

Cubic

Cubic

Crystallite size (nm)

20–62

23–48

21–53

16–40

14–29

9–29

Magnetization (emu/g)

10.4–27.9

15.2–40.4

9.9–46.8

5.0–38.1

1.3–20.4

Coercivity (Oe)

3.6–17.5

7.5–33.3

8.6–39.4

7.3–35.9

6.9–30.5

Navigation