Table 1 Yield, size, and zeta potential of SS-capped AgNPs synthesized from SS and AgNO 3 at pH 11
From: Green synthesis of silk sericin-capped silver nanoparticles and their potent anti-bacterial activity
Sample | Yield of AgNPs (mM) | Size (nm) | Zeta potential (mV) |
---|---|---|---|
5 mg/mL SS + 1 mM AgNO3 | 0.06 | 95.8 ± 0.9 | −23.7 ± 0.6 |
5 mg/mL SS + 5 mM AgNO3 | 0.75 | 48.8 ± 0.1* | −25.2 ± 0.2 |
5 mg/mL SS + 10 mM AgNO3 | 0.88 | 55.2 ± 0.6* | −17.1 ± 0.6 |
10 mg/mL SS + 1 mM AgNO3 | 0.04 | 117.0 ± 6.8 | −22.0 ± 0.1 |
10 mg/mL SS + 5 mM AgNO3 | 0.66 | 48.1 ± 0.2* | −25.5 ± 0.9 |
10 mg/mL SS + 10 mM AgNO3 | 0.93 | 63.6 ± 1.6* | −18.8 ± 2.3 |