Table 1 The UV emission spectra of a single ZnO microstructure and length and diameters of top end and bottom of the ZnO microstructure at different cooling times

From: Self-Etching-Induced Morphological Evolution of ZnO Microrods Grown on FTO Glass by Hydrothermal Method

Product (h)

PL peak1 (eV)

PL peak2 (eV)

Intensity ratio (peak2/peak1)

Length (μm)

Top-end diameter (μm)

Bottom diameter (μm)

1

3.22

3.29

0.216

8.89

0.80

1.23

2

3.20

3.32

0.331

8.63

0.86

1.23

3

3.20

3.32

0.251

7.25

0.90

1.22

4

3.20

3.32

0.364

7.00

0.91

1.23

5

3.20

3.32

0.187

6.69

0.92

1.23

6

3.21

3.30

0.490

6.49

0.93

1.12