Table 3 Viscosity measurement at 120 °C
From: Enhanced thermophysical properties via PAO superstructure
Shear rate (1/s) | PAO-1 | PAO-2 | PAO-3 | PAO + silica (1%) + PBP (1%)-1 | PAO + silica (1%) + PBP (1%)-2 | PAO + silica (1%) + PBP (1%)-3 |
---|---|---|---|---|---|---|
100 | 7.91 | 7.87 | 7.92 | 10.67 | 10.66 | 10.66 |
126 | 7.94 | 7.94 | 7.94 | 10.59 | 10.60 | 10.55 |
158 | 8.04 | 8.01 | 7.99 | 10.48 | 10.52 | 10.45 |
200 | 8.04 | 8.01 | 8.04 | 10.35 | 10.36 | 10.33 |
251 | 8.06 | 8.04 | 8.07 | 10.22 | 10.22 | 10.20 |
316 | 8.08 | 8.06 | 8.09 | 10.07 | 10.09 | 10.08 |
398 | 8.10 | 8.09 | 8.11 | 9.94 | 9.98 | 9.97 |
501 | 8.12 | 8.11 | 8.13 | 9.84 | 9.89 | 9.87 |
631 | 8.15 | 8.12 | 8.15 | 9.77 | 9.81 | 9.77 |
794 | 8.19 | 8.14 | 8.16 | 9.71 | 9.76 | 9.71 |
1000 | 8.24 | 8.19 | 8.20 | 9.67 | 9.71 | 9.63 |