Table 2 Weight losses (in wt%) of the PS/PANI-LSA nanocomposites (see Table 1), control PS nanoparticles, and SLS samples at different temperatures. LSA contents are given in brackets

From: New nanocomposites of polystyrene with polyaniline doped with lauryl sulfuric acid

Temperature, °C

NC2 (1.09)

NC3 (1.77)

NC11 (6.38)

NC15 (8.24)

PS

SLS

120

0.12

0.12

0.18

0.9

~0

0.61

180

0.96

0.64

0.85

2.12

0.8

1.29

208

1.33

1.33

1.33

2.93

1.33

3.92

262

3.45

4.59

7.64

8.78

1.93

39.98

290

5.68

5.68

8.74

10.27

5.68

58.06

330

7.04

6.65

12.01

12.01

9.33

70.50

350

7.83

7.06

15.86

15.86

12.80

71.00

430

69.42

50.68

83.56

80.50

82.04

72.86

505

99.42

98.65

91.01

83.36

97.5

73.04